PLASTIC FAMILY · ISO 1043: PA66

Polyamide 66 (Nylon 66) (PA66)

ISO 1043: PA66 · Polyamide · Semi-crystalline · Variants: Unreinforced PA66, PA66-GF30, Heat-Stabilized, MoS2 Wear Grade

High-melting semi-crystalline engineering polyamide offering high tensile strength, wear resistance, and strong tolerance to hydrocarbons, oils, and ketones.

Engineering Thermoplastic PA66 ISO 1043: PA66 Semi-crystalline
Density
1.13 – 1.15 g/cm³
Tensile Strength
70 – 85 MPa
Flexural Modulus
2600 – 3100 MPa
Max Service Temp
100 – 120 °C
Melting Point (Tm)
255 – 265 °C
PROPERTY BENCHMARKING

Key Mechanical & Thermal Comparison

PA66 typical range Category range Database median
Density 1.13 – 1.15 g/cm³ (0.0408 – 0.0415 lb/in³)
0.85 g/cm³ Cat: 1.13 – 1.22 · Median: 1.05 1.3 g/cm³
Tensile Strength 70 – 85 MPa (10,150 – 12,330 psi)
15 MPa Cat: 55 – 85 · Median: 50 95 MPa
Flexural Modulus 2600 – 3100 MPa (377 – 450 ksi)
500 MPa Cat: 2100 – 3100 · Median: 2200 3500 MPa
HDT @ 0.45 MPa 190 – 220 °C (374 – 428 °F)
50 °C Cat: 135 – 220 · Median: 105 240 °C
Max Continuous Service Temp 100 – 120 °C (212 – 248 °F)
50 °C Cat: 100 – 125 · Median: 100 150 °C

Source: ISO 1043 / MatWeb / Public Polyamide Resin Datasheets (Dry-as-Molded) · Retrieved 2026-11-24 · Ranges represent unreinforced injection-molding grades unless noted

MATERIAL PROPERTIES

Typical Engineering Property Ranges

Polyamide 66 (Nylon 66) property ranges
Property Typical Range (SI / Imperial)
Density 1.13 – 1.15 g/cm³ (0.0408 – 0.0415 lb/in³)
Tensile Strength (Yield / Break) 70 – 85 MPa (10,150 – 12,330 psi)
Flexural Modulus 2600 – 3100 MPa (377 – 450 ksi)
Elongation at Break 20 – 60 %
Notched Izod Impact (23 °C) 40 – 65 J/m (0.75 – 1.22 ft·lb/in)
HDT @ 0.45 MPa 190 – 220 °C (374 – 428 °F)
HDT @ 1.80 MPa 65 – 85 °C (149 – 185 °F)
Melting Point (Tm) 255 – 265 °C (491 – 509 °F)
Max Continuous Service Temp 100 – 120 °C (212 – 248 °F)
Water Absorption (24 h, 23 °C) 1 – 1.5 %

Source: ISO 1043 / MatWeb / Public Polyamide Resin Datasheets (Dry-as-Molded) · Retrieved 2026-11-24

MANUFACTURING & MOLDING

Processing Parameters

Polyamide 66 (Nylon 66) processing parameters
Parameter Recommended Range
Melt Temperature 270 – 300 °C (518 – 572 °F)
Mold Temperature 60 – 90 °C (140 – 194 °F)
Drying Temperature 80 – 85 °C (176 – 185 °F)
Drying Time 4 – 6 h (desiccant)
Injection Pressure 75 – 135 MPa (10,880 – 19,580 psi)
Mold Shrinkage 1.2 – 2 %
Common Molding Processes Injection molding, Extrusion, Compounding (glass-filled)

Source: ISO 1043 / MatWeb / Public Polyamide Resin Datasheets (Dry-as-Molded) · Retrieved 2026-11-24

APPLICATIONS & SELECTION

Typical Uses, Strengths & Limitations

Typical Industrial Applications
  • Under-hood automotive connectors, radiator end tanks, and intake manifolds
  • Gears, bushings, cams, and low-friction mechanical wear components
  • Cable ties, electrical terminal blocks, and coil bobbins
  • Industrial fastener clips and structural brackets (especially GF30 grades)
Key Advantages
  • High dry-as-molded tensile strength (70 – 85 MPa) and high melting point (260 °C)
  • Excellent resistance to hydrocarbons, fuels, lubricants, and ketones
  • Low coefficient of friction and high abrasion resistance
  • Strong property uplift with 15% – 50% glass fiber reinforcement
Design Limitations
  • Hygroscopic: absorbs 1.0 – 1.5% water in 24 h (up to ~8% saturation), shifting dimensions and modulus
  • Rapidly degraded by strong mineral acids (such as concentrated HCl)
  • Requires controlled desiccant drying prior to injection molding
  • Higher mold shrinkage (1.2 – 2.0%) than amorphous polymers

Source: ISO 1043 / MatWeb / Public Polyamide Resin Datasheets (Dry-as-Molded) · Retrieved 2026-11-24

CHEMICAL RESISTANCE

Common Chemicals vs. PA66

View full matrix →
PA66 resistance to common chemicals
Chemical (CAS) Rating & Conditions Engineering Notes
Acetone
CAS 67-64-1 · C3H6O
A Excellent 20 °C · 100% · Continuous immersion Polyamide 66 exhibits strong resistance to neat ketones including acetone at ambient temperature.
Ethanol
CAS 64-17-5 · C2H6O
B Good 20 °C · 96 – 100% · Continuous immersion Slight alcohol absorption and minor swelling/plasticization similar to moisture uptake; acceptable for most non-precision parts.
Toluene
CAS 108-88-3 · C7H8
A Excellent 20 °C · 100% · Continuous immersion Excellent resistance to aromatic hydrocarbons including toluene at ambient temperature.
Hydrochloric Acid (37%)
CAS 7647-01-0 · HCl
D Not recommended 20 °C · 37% aqueous · Short-term contact Severe attack; strong mineral acids rapidly hydrolyze amide bonds and dissolve PA66.
Sodium Hydroxide
CAS 1310-73-2 · NaOH
NR No data No verified test basis No data: published chemical resistance tables diverge for concentrated 50% NaOH on PA66 depending on moisture state and heat-stabilizer package; verify via coupon test.
Ethyl Acetate
CAS 141-78-6 · C4H8O2
NR No data No verified test basis No data: standard public reference charts lack consistent verified data for anhydrous ethyl acetate on unreinforced PA66; perform application immersion test.

Source: Cole-Parmer / Plastics Design Library · Retrieved 2026-11-24