PLASTIC FAMILY · ISO 1629: FKM

Fluoroelastomer (Viton) (FKM)

ISO 1629: FKM · Fluoroelastomer · Amorphous · Variants: Type A (66% Fluorine), Type B / F (68–70% Fluorine), GLT (Low-Temp), Peroxide-Cured

High-performance fluorinated synthetic rubber (widely known as Viton) offering up to 200 °C continuous sealing performance and superior resistance to oils, fuels, aromatics, chlorinated solvents, and strong mineral acids.

Industrial Elastomer FKM ISO 1629: FKM Amorphous
Density
1.8 – 1.95 g/cm³
Tensile Strength
10 – 18 MPa
Flexural Modulus
8 – 30 MPa
Max Service Temp
190 – 205 °C
Glass Transition (Tg)
-25 – -15 °C
PROPERTY BENCHMARKING

Key Mechanical & Thermal Comparison

FKM typical range Category range Database median
Density 1.8 – 1.95 g/cm³ (0.0650 – 0.0704 lb/in³)
0.85 g/cm³ Cat: 1.05 – 1.95 · Median: 1.2 2.25 g/cm³
Tensile Strength 10 – 18 MPa (1,450 – 2,610 psi)
5 MPa Cat: 6 – 22 · Median: 46 115 MPa
Flexural Modulus 8 – 30 MPa (1.2 – 4.4 ksi)
0 MPa Cat: 3 – 30 · Median: 2250 4400 MPa
Max Continuous Service Temp 190 – 205 °C (374 – 401 °F)
50 °C Cat: 95 – 210 · Median: 100 270 °C

Source: ISO 1629 / Chemours Viton / Parker O-Ring Handbook · Retrieved 2026-11-25 · Ranges represent unreinforced injection-molding grades unless noted

MATERIAL PROPERTIES

Typical Engineering Property Ranges

Fluoroelastomer (Viton) property ranges
Property Typical Range (SI / Imperial)
Density 1.8 – 1.95 g/cm³ (0.0650 – 0.0704 lb/in³)
Tensile Strength (Yield / Break) 10 – 18 MPa (1,450 – 2,610 psi)
Flexural Modulus 8 – 30 MPa (1.2 – 4.4 ksi)
Elongation at Break 150 – 300 %
Notched Izod Impact (23 °C) —
HDT @ 0.45 MPa —
HDT @ 1.80 MPa —
Glass Transition (Tg) -25 – -15 °C (-13 – 5 °F)
Max Continuous Service Temp 190 – 205 °C (374 – 401 °F)
Water Absorption (24 h, 23 °C) 0.1 – 0.5 %

Source: ISO 1629 / Chemours Viton / Parker O-Ring Handbook · Retrieved 2026-11-25

MANUFACTURING & MOLDING

Processing Parameters

Fluoroelastomer (Viton) processing parameters
Parameter Recommended Range
Melt Temperature 170 – 195 °C (338 – 383 °F)
Mold Temperature 170 – 190 °C (338 – 374 °F)
Drying Temperature —
Drying Time —
Injection Pressure 60 – 120 MPa (8,700 – 17,400 psi)
Mold Shrinkage 2 – 3.5 %
Common Molding Processes Compression molding, Transfer molding, Rubber injection molding, Extrusion

Source: ISO 1629 / Chemours Viton / Parker O-Ring Handbook · Retrieved 2026-11-25

APPLICATIONS & SELECTION

Typical Uses, Strengths & Limitations

Typical Industrial Applications
  • Chemical process pump mechanical seal O-rings and valve stem packings
  • Fuel injection seals, refinery hydrocarbon gaskets, and aerospace shaft seals
  • Concentrated mineral acid (H2SO4, HNO3, HCl) transfer seals
  • High-vacuum and high-temperature industrial flange seals
Key Advantages
  • Exceptional resistance to hydrocarbons, fuels, aromatics (toluene/xylene), oils, and concentrated mineral acids
  • Continuous thermal stability up to 200 °C with low compression set and low gas permeability
  • Self-extinguishing and immune to ozone, UV, and atmospheric oxidation
Design Limitations
  • Severely swelled and degraded by ketones (acetone, MEK), low-molecular-weight esters, THF, DMF, NMP, amines, and hot steam/caustics
  • Limited low-temperature flexibility (~-20 °C for standard Type A)
  • Higher material cost than NBR or EPDM

Source: ISO 1629 / Chemours Viton / Parker O-Ring Handbook · Retrieved 2026-11-25

CHEMICAL RESISTANCE

Common Chemicals vs. FKM

View full matrix →
FKM resistance to common chemicals
Chemical (CAS) Rating & Conditions Engineering Notes
Acetone
CAS 67-64-1 · C3H6O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Acetone causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Ethanol
CAS 64-17-5 · C2H6O
B Good 20 °C · 96 – 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Ethanol at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Toluene
CAS 108-88-3 · C7H8
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Toluene at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Hydrochloric Acid (37%)
CAS 7647-01-0 · HCl
A Excellent 20 °C · 37% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Hydrochloric Acid (37%) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Sodium Hydroxide
CAS 1310-73-2 · NaOH
B Good 20 °C · 40 – 50% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Sodium Hydroxide at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Ethyl Acetate
CAS 141-78-6 · C4H8O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Ethyl Acetate causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Methanol
CAS 67-56-1 · CH4O
C Fair 20 °C · 100% · Limited / intermittent contact
Manufacturer Ref · Ref chart ↗
Limited resistance to Methanol at 20 °C; moderate swelling, softening, or stress-cracking risk makes FKM (Viton) fluoroelastomer unsuitable for continuous containment.
Isopropanol (IPA)
CAS 67-63-0 · C3H8O
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Isopropanol (IPA) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Ethylene Glycol
CAS 107-21-1 · C2H6O2
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Ethylene Glycol at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
1-Butanol
CAS 71-36-3 · C4H10O
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to 1-Butanol at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Methyl Ethyl Ketone (MEK)
CAS 78-93-3 · C4H8O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl Ethyl Ketone (MEK) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Tetrahydrofuran (THF)
CAS 109-99-9 · C4H8O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Tetrahydrofuran (THF) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
n-Butyl Acetate
CAS 123-86-4 · C6H12O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: n-Butyl Acetate causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
n-Hexane
CAS 110-54-3 · C6H14
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to n-Hexane at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Cyclohexane
CAS 110-82-7 · C6H12
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Cyclohexane at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Styrene
CAS 100-42-5 · C8H8
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Styrene at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Dichloromethane (DCM)
CAS 75-09-2 · CH2Cl2
B Good 20 °C · 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Dichloromethane (DCM) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Chloroform
CAS 67-66-3 · CHCl3
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Chloroform at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
N,N-Dimethylformamide (DMF)
CAS 68-12-2 · C3H7NO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: N,N-Dimethylformamide (DMF) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Dimethyl Sulfoxide (DMSO)
CAS 67-68-5 · C2H6OS
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Dimethyl Sulfoxide (DMSO) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
N-Methyl-2-pyrrolidone (NMP)
CAS 872-50-4 · C5H9NO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: N-Methyl-2-pyrrolidone (NMP) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Sulfuric Acid (98%)
CAS 7664-93-9 · H2O4S
A Excellent 20 °C · 98% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sulfuric Acid (98%) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Nitric Acid (65%)
CAS 7697-37-2 · HNO3
A Excellent 20 °C · 65% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Nitric Acid (65%) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Phosphoric Acid (85%)
CAS 7664-38-2 · H3O4P
A Excellent 20 °C · 85% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Phosphoric Acid (85%) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Hydrogen Peroxide (30%)
CAS 7722-84-1 · H2O2
A Excellent 20 °C · 30% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Hydrogen Peroxide (30%) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Sodium Hypochlorite (12.5%)
CAS 7681-52-9 · ClNaO
A Excellent 20 °C · 12.5% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Hypochlorite (12.5%) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Acetic Acid (Glacial)
CAS 64-19-7 · C2H4O2
C Fair 20 °C · 100% (Glacial) · Limited / intermittent contact
Manufacturer Ref · Ref chart ↗
Limited resistance to Acetic Acid (Glacial) at 20 °C; moderate swelling, softening, or stress-cracking risk makes FKM (Viton) fluoroelastomer unsuitable for continuous containment.
Formic Acid (85%)
CAS 64-18-6 · CH2O2
C Fair 20 °C · 85% · Limited / intermittent contact
Manufacturer Ref · Ref chart ↗
Limited resistance to Formic Acid (85%) at 20 °C; moderate swelling, softening, or stress-cracking risk makes FKM (Viton) fluoroelastomer unsuitable for continuous containment.
Potassium Hydroxide (KOH)
CAS 1310-58-3 · HKO
B Good 20 °C · 45 – 50% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Potassium Hydroxide (KOH) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Ammonium Hydroxide (25%)
CAS 1336-21-6 · H5NO
B Good 20 °C · 25% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Ammonium Hydroxide (25%) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Methyl Isobutyl Ketone (MIBK)
CAS 108-10-1 · C6H12O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl Isobutyl Ketone (MIBK) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Cyclohexanone
CAS 108-94-1 · C6H10O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Cyclohexanone causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Methyl Acetate
CAS 79-20-9 · C3H6O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl Acetate causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Isopropyl Acetate
CAS 108-21-4 · C5H10O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Isopropyl Acetate causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
PGMEA (PMA)
CAS 108-65-6 · C6H12O3
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: PGMEA (PMA) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Diethyl Ether
CAS 60-29-7 · C4H10O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Diethyl Ether causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Methyl tert-Butyl Ether (MTBE)
CAS 1634-04-4 · C5H12O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl tert-Butyl Ether (MTBE) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
1,4-Dioxane
CAS 123-91-1 · C4H8O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: 1,4-Dioxane causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Benzene
CAS 71-43-2 · C6H6
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Benzene at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Ethylbenzene
CAS 100-41-4 · C8H10
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Ethylbenzene at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
p-Xylene
CAS 106-42-3 · C8H10
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to p-Xylene at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
n-Heptane
CAS 142-82-5 · C7H16
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to n-Heptane at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
n-Pentane
CAS 109-66-0 · C5H12
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to n-Pentane at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Trichloroethylene (TCE)
CAS 79-01-6 · C2HCl3
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Trichloroethylene (TCE) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Tetrachloroethylene (PCE)
CAS 127-18-4 · C2Cl4
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Tetrachloroethylene (PCE) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Acetonitrile
CAS 75-05-8 · C2H3N
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Acetonitrile causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Propylene Glycol (PG)
CAS 57-55-6 · C3H8O2
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Propylene Glycol (PG) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Glycerol (Glycerin)
CAS 56-81-5 · C3H8O3
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Glycerol (Glycerin) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Diethylene Glycol (DEG)
CAS 111-46-6 · C4H10O3
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Diethylene Glycol (DEG) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
2-Butoxyethanol
CAS 111-76-2 · C6H14O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: 2-Butoxyethanol causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Benzyl Alcohol
CAS 100-51-6 · C7H8O
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Benzyl Alcohol at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Isobutanol
CAS 78-83-1 · C4H10O
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Isobutanol at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
1-Propanol
CAS 71-23-8 · C3H8O
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to 1-Propanol at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Phenol
CAS 108-95-2 · C6H6O
A Excellent 20 °C · 90 – 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Phenol at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Bisphenol A (BPA)
CAS 80-05-7 · C15H16O2
A Excellent 20 °C · Solid / Aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Bisphenol A (BPA) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Methyl Methacrylate (MMA)
CAS 80-62-6 · C5H8O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl Methacrylate (MMA) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Acrylic Acid
CAS 79-10-7 · C3H4O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Acrylic Acid causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
n-Butyl Acrylate
CAS 141-32-2 · C7H12O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: n-Butyl Acrylate causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Vinyl Acetate Monomer (VAM)
CAS 108-05-4 · C4H6O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Vinyl Acetate Monomer (VAM) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Acrylonitrile
CAS 107-13-1 · C3H3N
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Acrylonitrile causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Caprolactam
CAS 105-60-2 · C6H11NO
B Good 20 °C · Solid / Aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Caprolactam at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Adipic Acid
CAS 124-04-9 · C6H10O4
A Excellent 20 °C · Solid / Aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Adipic Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Terephthalic Acid (PTA)
CAS 100-21-0 · C8H6O4
A Excellent 20 °C · Solid · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Terephthalic Acid (PTA) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Phthalic Anhydride
CAS 85-44-9 · C8H4O3
A Excellent 20 °C · Solid · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Phthalic Anhydride at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Maleic Anhydride
CAS 108-31-6 · C4H2O3
C Fair 20 °C · Solid / Aq. · Limited / intermittent contact
Manufacturer Ref · Ref chart ↗
Limited resistance to Maleic Anhydride at 20 °C; moderate swelling, softening, or stress-cracking risk makes FKM (Viton) fluoroelastomer unsuitable for continuous containment.
Epichlorohydrin (ECH)
CAS 106-89-8 · C3H5ClO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Epichlorohydrin (ECH) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Dioctyl Phthalate (DOP / DEHP)
CAS 117-81-7 · C24H38O4
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Dioctyl Phthalate (DOP / DEHP) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Dioctyl Terephthalate (DOTP)
CAS 6422-86-2 · C24H38O4
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Dioctyl Terephthalate (DOTP) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Dibutyl Phthalate (DBP)
CAS 84-74-2 · C16H22O4
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Dibutyl Phthalate (DBP) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Dioctyl Adipate (DOA)
CAS 103-23-1 · C22H42O4
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Dioctyl Adipate (DOA) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Acetyl Tributyl Citrate (ATBC)
CAS 77-90-7 · C20H34O8
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Acetyl Tributyl Citrate (ATBC) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Citric Acid
CAS 77-92-9 · C6H8O7
A Excellent 20 °C · 10 – 50% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Citric Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Oxalic Acid
CAS 144-62-7 · C2H2O4
A Excellent 20 °C · 10% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Oxalic Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Lactic Acid
CAS 50-21-5 · C3H6O3
A Excellent 20 °C · 85% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Lactic Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Benzoic Acid
CAS 65-85-0 · C7H6O2
A Excellent 20 °C · Solid / Sat. aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Benzoic Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Formaldehyde (37% Formalin)
CAS 50-00-0 · CH2O
A Excellent 20 °C · 37% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Formaldehyde (37% Formalin) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Glutaraldehyde (50%)
CAS 111-30-8 · C5H8O2
A Excellent 20 °C · 50% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Glutaraldehyde (50%) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
N,N-Dimethylacetamide (DMAc)
CAS 127-19-5 · C4H9NO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: N,N-Dimethylacetamide (DMAc) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Monoethanolamine (MEA)
CAS 141-43-5 · C2H7NO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Monoethanolamine (MEA) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Triethanolamine (TEA)
CAS 102-71-6 · C6H15NO3
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Triethanolamine (TEA) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Triethylamine (Et3N)
CAS 121-44-8 · C6H15N
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Triethylamine (Et3N) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Aniline
CAS 62-53-3 · C6H7N
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Aniline causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Ethylenediamine (EDA)
CAS 107-15-3 · C2H8N2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Ethylenediamine (EDA) causes rapid swelling, softening, and seal failure in FKM (Viton) fluoroelastomer; consider EPDM or PTFE/FEP-encapsulated seals instead.
Urea
CAS 57-13-6 · CH4N2O
A Excellent 20 °C · 32.5% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Urea at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Hydrofluoric Acid (48% HF)
CAS 7664-39-3 · FH
A Excellent 20 °C · 48% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Hydrofluoric Acid (48% HF) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Perchloric Acid (70%)
CAS 7601-90-3 · ClHO4
A Excellent 20 °C · 70% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Perchloric Acid (70%) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Boric Acid
CAS 10043-35-3 · BH3O3
A Excellent 20 °C · Sat. aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Boric Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Sodium Carbonate (Soda Ash)
CAS 497-19-8 · CNa2O3
A Excellent 20 °C · 20% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Carbonate (Soda Ash) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Sodium Bicarbonate
CAS 144-55-8 · CHNaO3
A Excellent 20 °C · Sat. aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Bicarbonate at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Sodium Chloride (Brine)
CAS 7647-14-5 · ClNa
A Excellent 20 °C · 26% brine · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Chloride (Brine) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Sodium Sulfate
CAS 7757-82-6 · Na2O4S
A Excellent 20 °C · Sat. aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Sulfate at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Calcium Chloride
CAS 10043-52-4 · CaCl2
A Excellent 20 °C · 35% brine · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Calcium Chloride at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Ferric Chloride (40% Solution)
CAS 7705-08-0 · Cl3Fe
A Excellent 20 °C · 40% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Ferric Chloride (40% Solution) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Copper(II) Sulfate
CAS 7758-98-7 · CuO4S
A Excellent 20 °C · Sat. aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Copper(II) Sulfate at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Potassium Permanganate
CAS 7722-64-7 · KMnO4
A Excellent 20 °C · 10% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Potassium Permanganate at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Calcium Hydroxide (Hydrated Lime)
CAS 1305-62-0 · CaH2O2
A Excellent 20 °C · Slurry · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Calcium Hydroxide (Hydrated Lime) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Sodium Lauryl Sulfate (SLS)
CAS 151-21-3 · C12H25NaO4S
A Excellent 20 °C · 30% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Lauryl Sulfate (SLS) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Titanium Dioxide (TiO2)
CAS 13463-67-7 · O2Ti
A Excellent 20 °C · Solid · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Titanium Dioxide (TiO2) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
Silicon Dioxide (Fumed Silica)
CAS 7631-86-9 · O2Si
A Excellent 20 °C · Solid · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Silicon Dioxide (Fumed Silica) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.
1,4-Butanediol (BDO)
CAS 110-63-4 · C4H10O2
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to 1,4-Butanediol (BDO) at 20 °C with negligible swelling, weight change, or mechanical degradation in FKM (Viton) fluoroelastomer.

Source: Parker O-Ring Handbook / Cole-Parmer Elastomer Compatibility Consensus · Retrieved 2026-11-25

SPECIFICATION-MATCHED SOURCING

Source FKM by Grade & Form Factor

FKM O-Rings & Flange Gaskets

Type A (66% Fluorine) · Chemical sealing grades

View Suppliers on Made-in-China.com
FKM Rubber Sheets, Hoses & Custom Molded Seals

Extruded tubing, sheets & custom rubber molding

View Suppliers on Made-in-China.com