PLASTIC FAMILY · ISO 1043: PS

Polystyrene (GPPS) (PS)

ISO 1043: PS · Styrenic · Amorphous · Variants: GPPS (General Purpose), HIPS (High Impact), EPS (Expandable), Medical Grade

Crystal-clear, rigid amorphous thermoplastic widely used in disposable laboratory ware, Petri dishes, optical housings, and rigid packaging where clarity and low cost are prioritized.

Commodity Thermoplastic PS ISO 1043: PS Amorphous
Density
1.04 – 1.06 g/cm³
Tensile Strength
38 – 55 MPa
Flexural Modulus
2800 – 3400 MPa
Max Service Temp
65 – 75 °C
Glass Transition (Tg)
95 – 105 °C
PROPERTY BENCHMARKING

Key Mechanical & Thermal Comparison

PS typical range Category range Database median
Density 1.04 – 1.06 g/cm³ (0.0376 – 0.0383 lb/in³)
0.85 g/cm³ Cat: 0.9 – 1.44 · Median: 1.2 2.25 g/cm³
Tensile Strength 38 – 55 MPa (5,510 – 7,980 psi)
5 MPa Cat: 10 – 60 · Median: 46 115 MPa
Flexural Modulus 2800 – 3400 MPa (406 – 493 ksi)
0 MPa Cat: 170 – 3400 · Median: 2250 4400 MPa
HDT @ 0.45 MPa 78 – 95 °C (172 – 203 °F)
35 °C Cat: 40 – 115 · Median: 99 245 °C
Max Continuous Service Temp 65 – 75 °C (149 – 167 °F)
50 °C Cat: 55 – 110 · Median: 100 270 °C

Source: ISO 1043 / MatWeb / Public Styrenic Resin Datasheets · Retrieved 2026-11-25 · Ranges represent unreinforced injection-molding grades unless noted

MATERIAL PROPERTIES

Typical Engineering Property Ranges

Polystyrene (GPPS) property ranges
Property Typical Range (SI / Imperial)
Density 1.04 – 1.06 g/cm³ (0.0376 – 0.0383 lb/in³)
Tensile Strength (Yield / Break) 38 – 55 MPa (5,510 – 7,980 psi)
Flexural Modulus 2800 – 3400 MPa (406 – 493 ksi)
Elongation at Break 1.5 – 3.5 %
Notched Izod Impact (23 °C) 15 – 25 J/m (0.28 – 0.47 ft·lb/in)
HDT @ 0.45 MPa 78 – 95 °C (172 – 203 °F)
HDT @ 1.80 MPa 70 – 85 °C (158 – 185 °F)
Glass Transition (Tg) 95 – 105 °C (203 – 221 °F)
Max Continuous Service Temp 65 – 75 °C (149 – 167 °F)
Water Absorption (24 h, 23 °C) 0.03 – 0.1 %

Source: ISO 1043 / MatWeb / Public Styrenic Resin Datasheets · Retrieved 2026-11-25

MANUFACTURING & MOLDING

Processing Parameters

Polystyrene (GPPS) processing parameters
Parameter Recommended Range
Melt Temperature 180 – 240 °C (356 – 464 °F)
Mold Temperature 20 – 60 °C (68 – 140 °F)
Drying Temperature —
Drying Time —
Injection Pressure 60 – 120 MPa (8,700 – 17,400 psi)
Mold Shrinkage 0.4 – 0.7 %
Common Molding Processes Injection molding, Sheet extrusion, Thermoforming

Source: ISO 1043 / MatWeb / Public Styrenic Resin Datasheets · Retrieved 2026-11-25

APPLICATIONS & SELECTION

Typical Uses, Strengths & Limitations

Typical Industrial Applications
  • Disposable Petri dishes, culture plates, cuvettes, and diagnostic housings
  • Rigid transparent food packaging and display cases
  • Electrical insulation components and light-diffuser panels
  • Office supplies and consumer appliance housings (HIPS grades)
Key Advantages
  • High optical clarity (~89% light transmission) and surface gloss
  • Low mold shrinkage and easy high-speed injection molding
  • Resistant to aqueous acids, alkalis, and dilute salt solutions
  • Very low moisture absorption and low resin cost
Design Limitations
  • Brittle under impact (use HIPS or ABS when toughness is required)
  • Poor chemical resistance to organic solvents (ketones, esters, aromatics, chlorinated hydrocarbons)
  • Low heat resistance (~70 °C continuous service) and susceptible to UV yellowing

Source: ISO 1043 / MatWeb / Public Styrenic Resin Datasheets · Retrieved 2026-11-25

CHEMICAL RESISTANCE

Common Chemicals vs. PS

View full matrix →
PS resistance to common chemicals
Chemical (CAS) Rating & Conditions Engineering Notes
Acetone
CAS 67-64-1 · C3H6O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: acetone causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Ethanol
CAS 64-17-5 · C2H6O
B Good 20 °C · 96 – 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to ethanol at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Toluene
CAS 108-88-3 · C7H8
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: toluene causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Hydrochloric Acid (37%)
CAS 7647-01-0 · HCl
A Excellent 20 °C · 37% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to 37% hydrochloric acid at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed polystyrene (PS).
Sodium Hydroxide
CAS 1310-73-2 · NaOH
B Good 20 °C · 40 – 50% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to concentrated sodium hydroxide at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Ethyl Acetate
CAS 141-78-6 · C4H8O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: ethyl acetate causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Methanol
CAS 67-56-1 · CH4O
B Good 20 °C · 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to methanol at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Isopropanol (IPA)
CAS 67-63-0 · C3H8O
B Good 20 °C · 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to isopropanol (IPA) at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Ethylene Glycol
CAS 107-21-1 · C2H6O2
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to ethylene glycol at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed polystyrene (PS).
1-Butanol
CAS 71-36-3 · C4H10O
B Good 20 °C · 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to 1-butanol at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Methyl Ethyl Ketone (MEK)
CAS 78-93-3 · C4H8O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: methyl ethyl ketone (MEK) causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Tetrahydrofuran (THF)
CAS 109-99-9 · C4H8O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: tetrahydrofuran (THF) causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
n-Butyl Acetate
CAS 123-86-4 · C6H12O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: n-butyl acetate causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
n-Hexane
CAS 110-54-3 · C6H14
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: n-hexane causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Cyclohexane
CAS 110-82-7 · C6H12
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: cyclohexane causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Styrene
CAS 100-42-5 · C8H8
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: styrene monomer causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Dichloromethane (DCM)
CAS 75-09-2 · CH2Cl2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: dichloromethane (DCM) causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Chloroform
CAS 67-66-3 · CHCl3
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: chloroform causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
N,N-Dimethylformamide (DMF)
CAS 68-12-2 · C3H7NO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: N,N-dimethylformamide (DMF) causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Dimethyl Sulfoxide (DMSO)
CAS 67-68-5 · C2H6OS
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: dimethyl sulfoxide (DMSO) causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
N-Methyl-2-pyrrolidone (NMP)
CAS 872-50-4 · C5H9NO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: N-methyl-2-pyrrolidone (NMP) causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Sulfuric Acid (98%)
CAS 7664-93-9 · H2O4S
D Not recommended 20 °C · 98% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: 98% sulfuric acid causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Nitric Acid (65%)
CAS 7697-37-2 · HNO3
D Not recommended 20 °C · 65% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: 65% nitric acid causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Phosphoric Acid (85%)
CAS 7664-38-2 · H3O4P
B Good 20 °C · 85% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to 85% phosphoric acid at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Hydrogen Peroxide (30%)
CAS 7722-84-1 · H2O2
B Good 20 °C · 30% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to 30% hydrogen peroxide at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Sodium Hypochlorite (12.5%)
CAS 7681-52-9 · ClNaO
B Good 20 °C · 12.5% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to 12.5% sodium hypochlorite at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Acetic Acid (Glacial)
CAS 64-19-7 · C2H4O2
D Not recommended 20 °C · 100% (Glacial) · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: glacial acetic acid causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Formic Acid (85%)
CAS 64-18-6 · CH2O2
D Not recommended 20 °C · 85% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: 85% formic acid causes severe chemical attack, dissolution, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Potassium Hydroxide (KOH)
CAS 1310-58-3 · HKO
B Good 20 °C · 45 – 50% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to concentrated potassium hydroxide (KOH) at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Ammonium Hydroxide (25%)
CAS 1336-21-6 · H5NO
B Good 20 °C · 25% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to 25% ammonium hydroxide at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature.
Methyl Isobutyl Ketone (MIBK)
CAS 108-10-1 · C6H12O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl Isobutyl Ketone (MIBK) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Cyclohexanone
CAS 108-94-1 · C6H10O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Cyclohexanone causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Methyl Acetate
CAS 79-20-9 · C3H6O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl Acetate causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Isopropyl Acetate
CAS 108-21-4 · C5H10O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Isopropyl Acetate causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
PGMEA (PMA)
CAS 108-65-6 · C6H12O3
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: PGMEA (PMA) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Diethyl Ether
CAS 60-29-7 · C4H10O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Diethyl Ether causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Methyl tert-Butyl Ether (MTBE)
CAS 1634-04-4 · C5H12O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl tert-Butyl Ether (MTBE) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
1,4-Dioxane
CAS 123-91-1 · C4H8O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: 1,4-Dioxane causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Benzene
CAS 71-43-2 · C6H6
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Benzene causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Ethylbenzene
CAS 100-41-4 · C8H10
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Ethylbenzene causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
p-Xylene
CAS 106-42-3 · C8H10
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: p-Xylene causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
n-Heptane
CAS 142-82-5 · C7H16
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: n-Heptane causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
n-Pentane
CAS 109-66-0 · C5H12
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: n-Pentane causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Trichloroethylene (TCE)
CAS 79-01-6 · C2HCl3
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Trichloroethylene (TCE) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Tetrachloroethylene (PCE)
CAS 127-18-4 · C2Cl4
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Tetrachloroethylene (PCE) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Acetonitrile
CAS 75-05-8 · C2H3N
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Acetonitrile causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Propylene Glycol (PG)
CAS 57-55-6 · C3H8O2
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Propylene Glycol (PG) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Glycerol (Glycerin)
CAS 56-81-5 · C3H8O3
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Glycerol (Glycerin) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Diethylene Glycol (DEG)
CAS 111-46-6 · C4H10O3
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Diethylene Glycol (DEG) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
2-Butoxyethanol
CAS 111-76-2 · C6H14O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: 2-Butoxyethanol causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Benzyl Alcohol
CAS 100-51-6 · C7H8O
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Benzyl Alcohol causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Isobutanol
CAS 78-83-1 · C4H10O
B Good 20 °C · 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Isobutanol at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
1-Propanol
CAS 71-23-8 · C3H8O
B Good 20 °C · 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to 1-Propanol at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Phenol
CAS 108-95-2 · C6H6O
D Not recommended 20 °C · 90 – 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Phenol causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Bisphenol A (BPA)
CAS 80-05-7 · C15H16O2
A Excellent 20 °C · Solid / Aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Bisphenol A (BPA) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Methyl Methacrylate (MMA)
CAS 80-62-6 · C5H8O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Methyl Methacrylate (MMA) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Acrylic Acid
CAS 79-10-7 · C3H4O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Acrylic Acid causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
n-Butyl Acrylate
CAS 141-32-2 · C7H12O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: n-Butyl Acrylate causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Vinyl Acetate Monomer (VAM)
CAS 108-05-4 · C4H6O2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Vinyl Acetate Monomer (VAM) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Acrylonitrile
CAS 107-13-1 · C3H3N
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Acrylonitrile causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Caprolactam
CAS 105-60-2 · C6H11NO
B Good 20 °C · Solid / Aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Caprolactam at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Adipic Acid
CAS 124-04-9 · C6H10O4
B Good 20 °C · Solid / Aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Adipic Acid at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Terephthalic Acid (PTA)
CAS 100-21-0 · C8H6O4
A Excellent 20 °C · Solid · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Terephthalic Acid (PTA) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Phthalic Anhydride
CAS 85-44-9 · C8H4O3
B Good 20 °C · Solid · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Phthalic Anhydride at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Maleic Anhydride
CAS 108-31-6 · C4H2O3
B Good 20 °C · Solid / Aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Maleic Anhydride at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Epichlorohydrin (ECH)
CAS 106-89-8 · C3H5ClO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Epichlorohydrin (ECH) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Dioctyl Phthalate (DOP / DEHP)
CAS 117-81-7 · C24H38O4
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Dioctyl Phthalate (DOP / DEHP) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Dioctyl Terephthalate (DOTP)
CAS 6422-86-2 · C24H38O4
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Dioctyl Terephthalate (DOTP) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Dibutyl Phthalate (DBP)
CAS 84-74-2 · C16H22O4
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Dibutyl Phthalate (DBP) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Dioctyl Adipate (DOA)
CAS 103-23-1 · C22H42O4
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Dioctyl Adipate (DOA) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Acetyl Tributyl Citrate (ATBC)
CAS 77-90-7 · C20H34O8
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Acetyl Tributyl Citrate (ATBC) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Citric Acid
CAS 77-92-9 · C6H8O7
B Good 20 °C · 10 – 50% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Citric Acid at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Oxalic Acid
CAS 144-62-7 · C2H2O4
B Good 20 °C · 10% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Oxalic Acid at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Lactic Acid
CAS 50-21-5 · C3H6O3
B Good 20 °C · 85% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Lactic Acid at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Benzoic Acid
CAS 65-85-0 · C7H6O2
B Good 20 °C · Solid / Sat. aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Benzoic Acid at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Formaldehyde (37% Formalin)
CAS 50-00-0 · CH2O
B Good 20 °C · 37% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Formaldehyde (37% Formalin) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Glutaraldehyde (50%)
CAS 111-30-8 · C5H8O2
B Good 20 °C · 50% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Glutaraldehyde (50%) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
N,N-Dimethylacetamide (DMAc)
CAS 127-19-5 · C4H9NO
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: N,N-Dimethylacetamide (DMAc) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Monoethanolamine (MEA)
CAS 141-43-5 · C2H7NO
B Good 20 °C · 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Monoethanolamine (MEA) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Triethanolamine (TEA)
CAS 102-71-6 · C6H15NO3
B Good 20 °C · 100% · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Triethanolamine (TEA) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Triethylamine (Et3N)
CAS 121-44-8 · C6H15N
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Triethylamine (Et3N) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Aniline
CAS 62-53-3 · C6H7N
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Aniline causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Ethylenediamine (EDA)
CAS 107-15-3 · C2H8N2
D Not recommended 20 °C · 100% · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Ethylenediamine (EDA) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Urea
CAS 57-13-6 · CH4N2O
A Excellent 20 °C · 32.5% aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Urea at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Hydrofluoric Acid (48% HF)
CAS 7664-39-3 · FH
B Good 20 °C · 48% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Hydrofluoric Acid (48% HF) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Perchloric Acid (70%)
CAS 7601-90-3 · ClHO4
D Not recommended 20 °C · 70% aq. · Short-term contact
Manufacturer Ref · Ref chart ↗
Not recommended: Perchloric Acid (70%) causes severe attack, swelling, crazing, or rapid structural failure in polystyrene (PS) even under short-term contact.
Boric Acid
CAS 10043-35-3 · BH3O3
A Excellent 20 °C · Sat. aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Boric Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Sodium Carbonate (Soda Ash)
CAS 497-19-8 · CNa2O3
B Good 20 °C · 20% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Sodium Carbonate (Soda Ash) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Sodium Bicarbonate
CAS 144-55-8 · CHNaO3
A Excellent 20 °C · Sat. aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Bicarbonate at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Sodium Chloride (Brine)
CAS 7647-14-5 · ClNa
A Excellent 20 °C · 26% brine · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Chloride (Brine) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Sodium Sulfate
CAS 7757-82-6 · Na2O4S
A Excellent 20 °C · Sat. aq. · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Sodium Sulfate at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Calcium Chloride
CAS 10043-52-4 · CaCl2
B Good 20 °C · 35% brine · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Calcium Chloride at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Ferric Chloride (40% Solution)
CAS 7705-08-0 · Cl3Fe
B Good 20 °C · 40% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Ferric Chloride (40% Solution) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Copper(II) Sulfate
CAS 7758-98-7 · CuO4S
B Good 20 °C · Sat. aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Copper(II) Sulfate at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Potassium Permanganate
CAS 7722-64-7 · KMnO4
B Good 20 °C · 10% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Potassium Permanganate at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Calcium Hydroxide (Hydrated Lime)
CAS 1305-62-0 · CaH2O2
B Good 20 °C · Slurry · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Calcium Hydroxide (Hydrated Lime) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Sodium Lauryl Sulfate (SLS)
CAS 151-21-3 · C12H25NaO4S
B Good 20 °C · 30% aq. · Ambient contact
Manufacturer Ref · Ref chart ↗
Good resistance to Sodium Lauryl Sulfate (SLS) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature.
Titanium Dioxide (TiO2)
CAS 13463-67-7 · O2Ti
A Excellent 20 °C · Solid · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Titanium Dioxide (TiO2) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
Silicon Dioxide (Fumed Silica)
CAS 7631-86-9 · O2Si
A Excellent 20 °C · Solid · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to Silicon Dioxide (Fumed Silica) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).
1,4-Butanediol (BDO)
CAS 110-63-4 · C4H10O2
A Excellent 20 °C · 100% · Continuous immersion
Manufacturer Ref · Ref chart ↗
Excellent resistance to 1,4-Butanediol (BDO) at 20 °C with negligible swelling, weight change, or mechanical degradation in polystyrene (PS).

Source: Cole-Parmer / Thermo Scientific (Nalgene) / GF Piping Consensus · Retrieved 2026-11-25

SPECIFICATION-MATCHED SOURCING

Source PS by Grade & Form Factor

PS Virgin & Modified Resin Pellets

GPPS (General Purpose) / HIPS (High Impact) · Injection & extrusion grades

View Suppliers on Made-in-China.com
PS Sheets, Rods & Custom Injection Molded Parts

Injection molding & Sheet extrusion manufacturers

View Suppliers on Made-in-China.com