Styrene-Acrylonitrile (SAN)
Transparent amorphous copolymer of styrene and acrylonitrile offering higher stiffness, heat deflection, and resistance to oils and fats than general-purpose polystyrene.
Key Mechanical & Thermal Comparison
Source: ISO 1043 / INEOS Styrolution / MatWeb Public Datasheets · Retrieved 2026-11-25 · Ranges represent unreinforced injection-molding grades unless noted
Typical Engineering Property Ranges
| Property | Typical Range (SI / Imperial) |
|---|---|
| Density | 1.07 – 1.09 g/cm³ (0.0387 – 0.0394 lb/in³) |
| Tensile Strength (Yield / Break) | 65 – 78 MPa (9,430 – 11,310 psi) |
| Flexural Modulus | 3400 – 3900 MPa (493 – 566 ksi) |
| Elongation at Break | 2 – 5 % |
| Notched Izod Impact (23 °C) | 20 – 30 J/m (0.37 – 0.56 ft·lb/in) |
| HDT @ 0.45 MPa | 95 – 103 °C (203 – 217 °F) |
| HDT @ 1.80 MPa | 85 – 96 °C (185 – 205 °F) |
| Glass Transition (Tg) | 105 – 112 °C (221 – 234 °F) |
| Max Continuous Service Temp | 75 – 85 °C (167 – 185 °F) |
| Water Absorption (24 h, 23 °C) | 0.2 – 0.35 % |
Source: ISO 1043 / INEOS Styrolution / MatWeb Public Datasheets · Retrieved 2026-11-25
Processing Parameters
| Parameter | Recommended Range |
|---|---|
| Melt Temperature | 200 – 250 °C (392 – 482 °F) |
| Mold Temperature | 40 – 80 °C (104 – 176 °F) |
| Drying Temperature | 75 – 85 °C (167 – 185 °F) |
| Drying Time | 2 – 4 h |
| Injection Pressure | 70 – 130 MPa (10,150 – 18,850 psi) |
| Mold Shrinkage | 0.3 – 0.6 % |
| Common Molding Processes | Injection molding, Extrusion, Blow molding |
Source: ISO 1043 / INEOS Styrolution / MatWeb Public Datasheets · Retrieved 2026-11-25
Typical Uses, Strengths & Limitations
- Water filter housings, sight bowls, and appliance pitchers
- Cosmetic jars, battery cases, and medical dialyzer housings
- Industrial instrument lenses and clear refrigerator drawers
- Higher tensile strength, modulus, and HDT than GPPS
- Better resistance to aliphatic hydrocarbons, greases, and detergents than PS
- High optical clarity (~88% transmission) and low mold shrinkage
- Relatively low notched impact resistance compared to ABS or PC
- Rapidly dissolved or crazed by ketones, esters, aromatic, and chlorinated solvents
- Prone to yellowing under prolonged outdoor UV exposure without stabilizers
Source: ISO 1043 / INEOS Styrolution / MatWeb Public Datasheets · Retrieved 2026-11-25
Common Chemicals vs. SAN
| Chemical (CAS) | Rating & Conditions | Engineering Notes |
|---|---|---|
| Acetone CAS 67-64-1 · C3H6O | Not recommended: acetone causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Ethanol CAS 64-17-5 · C2H6O | Good resistance to ethanol at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature. | |
| Toluene CAS 108-88-3 · C7H8 | Not recommended: toluene causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Hydrochloric Acid (37%) CAS 7647-01-0 · HCl | Excellent resistance to 37% hydrochloric acid at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Sodium Hydroxide CAS 1310-73-2 · NaOH | Excellent resistance to concentrated sodium hydroxide at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Ethyl Acetate CAS 141-78-6 · C4H8O2 | Not recommended: ethyl acetate causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Methanol CAS 67-56-1 · CH4O | Good resistance to methanol at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature. | |
| Isopropanol (IPA) CAS 67-63-0 · C3H8O | Good resistance to isopropanol (IPA) at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature. | |
| Ethylene Glycol CAS 107-21-1 · C2H6O2 | Excellent resistance to ethylene glycol at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| 1-Butanol CAS 71-36-3 · C4H10O | Good resistance to 1-butanol at 20 °C; minor absorption, slight swelling, or gradual property change possible over prolonged exposure or elevated temperature. | |
| Methyl Ethyl Ketone (MEK) CAS 78-93-3 · C4H8O | Not recommended: methyl ethyl ketone (MEK) causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Tetrahydrofuran (THF) CAS 109-99-9 · C4H8O | Not recommended: tetrahydrofuran (THF) causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| n-Butyl Acetate CAS 123-86-4 · C6H12O2 | Not recommended: n-butyl acetate causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| n-Hexane CAS 110-54-3 · C6H14 | Limited resistance to n-hexane at 20 °C; moderate swelling, softening, or stress-cracking risk makes SAN unsuitable for continuous pressurized containment. | |
| Cyclohexane CAS 110-82-7 · C6H12 | Limited resistance to cyclohexane at 20 °C; moderate swelling, softening, or stress-cracking risk makes SAN unsuitable for continuous pressurized containment. | |
| Styrene CAS 100-42-5 · C8H8 | Not recommended: styrene monomer causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Dichloromethane (DCM) CAS 75-09-2 · CH2Cl2 | Not recommended: dichloromethane (DCM) causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Chloroform CAS 67-66-3 · CHCl3 | Not recommended: chloroform causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| N,N-Dimethylformamide (DMF) CAS 68-12-2 · C3H7NO | Not recommended: N,N-dimethylformamide (DMF) causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Dimethyl Sulfoxide (DMSO) CAS 67-68-5 · C2H6OS | Not recommended: dimethyl sulfoxide (DMSO) causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| N-Methyl-2-pyrrolidone (NMP) CAS 872-50-4 · C5H9NO | Not recommended: N-methyl-2-pyrrolidone (NMP) causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Sulfuric Acid (98%) CAS 7664-93-9 · H2O4S | Not recommended: 98% sulfuric acid causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Nitric Acid (65%) CAS 7697-37-2 · HNO3 | Not recommended: 65% nitric acid causes severe chemical attack, dissolution, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Phosphoric Acid (85%) CAS 7664-38-2 · H3O4P | Excellent resistance to 85% phosphoric acid at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Hydrogen Peroxide (30%) CAS 7722-84-1 · H2O2 | Excellent resistance to 30% hydrogen peroxide at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Sodium Hypochlorite (12.5%) CAS 7681-52-9 · ClNaO | Excellent resistance to 12.5% sodium hypochlorite at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Acetic Acid (Glacial) CAS 64-19-7 · C2H4O2 | Excellent resistance to glacial acetic acid at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Formic Acid (85%) CAS 64-18-6 · CH2O2 | Excellent resistance to 85% formic acid at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Potassium Hydroxide (KOH) CAS 1310-58-3 · HKO | Excellent resistance to concentrated potassium hydroxide (KOH) at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Ammonium Hydroxide (25%) CAS 1336-21-6 · H5NO | Excellent resistance to 25% ammonium hydroxide at 20 °C with negligible swelling, weight change, or mechanical loss in unstressed SAN. | |
| Methyl Isobutyl Ketone (MIBK) CAS 108-10-1 · C6H12O | Not recommended: Methyl Isobutyl Ketone (MIBK) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Cyclohexanone CAS 108-94-1 · C6H10O | Not recommended: Cyclohexanone causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Methyl Acetate CAS 79-20-9 · C3H6O2 | Not recommended: Methyl Acetate causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Isopropyl Acetate CAS 108-21-4 · C5H10O2 | Not recommended: Isopropyl Acetate causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| PGMEA (PMA) CAS 108-65-6 · C6H12O3 | Not recommended: PGMEA (PMA) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Diethyl Ether CAS 60-29-7 · C4H10O | Not recommended: Diethyl Ether causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Methyl tert-Butyl Ether (MTBE) CAS 1634-04-4 · C5H12O | Not recommended: Methyl tert-Butyl Ether (MTBE) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| 1,4-Dioxane CAS 123-91-1 · C4H8O2 | Not recommended: 1,4-Dioxane causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Benzene CAS 71-43-2 · C6H6 | Not recommended: Benzene causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Ethylbenzene CAS 100-41-4 · C8H10 | Not recommended: Ethylbenzene causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| p-Xylene CAS 106-42-3 · C8H10 | Not recommended: p-Xylene causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| n-Heptane CAS 142-82-5 · C7H16 | Limited resistance to n-Heptane at 20 °C; moderate swelling, softening, or stress-cracking risk makes SAN unsuitable for continuous containment. | |
| n-Pentane CAS 109-66-0 · C5H12 | Limited resistance to n-Pentane at 20 °C; moderate swelling, softening, or stress-cracking risk makes SAN unsuitable for continuous containment. | |
| Trichloroethylene (TCE) CAS 79-01-6 · C2HCl3 | Not recommended: Trichloroethylene (TCE) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Tetrachloroethylene (PCE) CAS 127-18-4 · C2Cl4 | Not recommended: Tetrachloroethylene (PCE) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Acetonitrile CAS 75-05-8 · C2H3N | Not recommended: Acetonitrile causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Propylene Glycol (PG) CAS 57-55-6 · C3H8O2 | Excellent resistance to Propylene Glycol (PG) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Glycerol (Glycerin) CAS 56-81-5 · C3H8O3 | Excellent resistance to Glycerol (Glycerin) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Diethylene Glycol (DEG) CAS 111-46-6 · C4H10O3 | Excellent resistance to Diethylene Glycol (DEG) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| 2-Butoxyethanol CAS 111-76-2 · C6H14O2 | Good resistance to 2-Butoxyethanol at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature. | |
| Benzyl Alcohol CAS 100-51-6 · C7H8O | Not recommended: Benzyl Alcohol causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Isobutanol CAS 78-83-1 · C4H10O | Good resistance to Isobutanol at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature. | |
| 1-Propanol CAS 71-23-8 · C3H8O | Good resistance to 1-Propanol at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature. | |
| Phenol CAS 108-95-2 · C6H6O | Not recommended: Phenol causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Bisphenol A (BPA) CAS 80-05-7 · C15H16O2 | Excellent resistance to Bisphenol A (BPA) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Methyl Methacrylate (MMA) CAS 80-62-6 · C5H8O2 | Not recommended: Methyl Methacrylate (MMA) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Acrylic Acid CAS 79-10-7 · C3H4O2 | Not recommended: Acrylic Acid causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| n-Butyl Acrylate CAS 141-32-2 · C7H12O2 | Not recommended: n-Butyl Acrylate causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Vinyl Acetate Monomer (VAM) CAS 108-05-4 · C4H6O2 | Not recommended: Vinyl Acetate Monomer (VAM) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Acrylonitrile CAS 107-13-1 · C3H3N | Not recommended: Acrylonitrile causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Caprolactam CAS 105-60-2 · C6H11NO | Excellent resistance to Caprolactam at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Adipic Acid CAS 124-04-9 · C6H10O4 | Excellent resistance to Adipic Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Terephthalic Acid (PTA) CAS 100-21-0 · C8H6O4 | Excellent resistance to Terephthalic Acid (PTA) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Phthalic Anhydride CAS 85-44-9 · C8H4O3 | Excellent resistance to Phthalic Anhydride at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Maleic Anhydride CAS 108-31-6 · C4H2O3 | Excellent resistance to Maleic Anhydride at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Epichlorohydrin (ECH) CAS 106-89-8 · C3H5ClO | Not recommended: Epichlorohydrin (ECH) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Dioctyl Phthalate (DOP / DEHP) CAS 117-81-7 · C24H38O4 | Not recommended: Dioctyl Phthalate (DOP / DEHP) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Dioctyl Terephthalate (DOTP) CAS 6422-86-2 · C24H38O4 | Not recommended: Dioctyl Terephthalate (DOTP) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Dibutyl Phthalate (DBP) CAS 84-74-2 · C16H22O4 | Not recommended: Dibutyl Phthalate (DBP) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Dioctyl Adipate (DOA) CAS 103-23-1 · C22H42O4 | Not recommended: Dioctyl Adipate (DOA) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Acetyl Tributyl Citrate (ATBC) CAS 77-90-7 · C20H34O8 | Not recommended: Acetyl Tributyl Citrate (ATBC) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Citric Acid CAS 77-92-9 · C6H8O7 | Excellent resistance to Citric Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Oxalic Acid CAS 144-62-7 · C2H2O4 | Excellent resistance to Oxalic Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Lactic Acid CAS 50-21-5 · C3H6O3 | Excellent resistance to Lactic Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Benzoic Acid CAS 65-85-0 · C7H6O2 | Excellent resistance to Benzoic Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Formaldehyde (37% Formalin) CAS 50-00-0 · CH2O | Excellent resistance to Formaldehyde (37% Formalin) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Glutaraldehyde (50%) CAS 111-30-8 · C5H8O2 | Excellent resistance to Glutaraldehyde (50%) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| N,N-Dimethylacetamide (DMAc) CAS 127-19-5 · C4H9NO | Not recommended: N,N-Dimethylacetamide (DMAc) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Monoethanolamine (MEA) CAS 141-43-5 · C2H7NO | Excellent resistance to Monoethanolamine (MEA) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Triethanolamine (TEA) CAS 102-71-6 · C6H15NO3 | Excellent resistance to Triethanolamine (TEA) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Triethylamine (Et3N) CAS 121-44-8 · C6H15N | Not recommended: Triethylamine (Et3N) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Aniline CAS 62-53-3 · C6H7N | Not recommended: Aniline causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Ethylenediamine (EDA) CAS 107-15-3 · C2H8N2 | Excellent resistance to Ethylenediamine (EDA) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Urea CAS 57-13-6 · CH4N2O | Excellent resistance to Urea at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Hydrofluoric Acid (48% HF) CAS 7664-39-3 · FH | Excellent resistance to Hydrofluoric Acid (48% HF) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Perchloric Acid (70%) CAS 7601-90-3 · ClHO4 | Not recommended: Perchloric Acid (70%) causes severe attack, swelling, crazing, or rapid structural failure in SAN even under short-term contact. | |
| Boric Acid CAS 10043-35-3 · BH3O3 | Excellent resistance to Boric Acid at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Sodium Carbonate (Soda Ash) CAS 497-19-8 · CNa2O3 | Excellent resistance to Sodium Carbonate (Soda Ash) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Sodium Bicarbonate CAS 144-55-8 · CHNaO3 | Excellent resistance to Sodium Bicarbonate at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Sodium Chloride (Brine) CAS 7647-14-5 · ClNa | Excellent resistance to Sodium Chloride (Brine) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Sodium Sulfate CAS 7757-82-6 · Na2O4S | Excellent resistance to Sodium Sulfate at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Calcium Chloride CAS 10043-52-4 · CaCl2 | Excellent resistance to Calcium Chloride at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Ferric Chloride (40% Solution) CAS 7705-08-0 · Cl3Fe | Excellent resistance to Ferric Chloride (40% Solution) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Copper(II) Sulfate CAS 7758-98-7 · CuO4S | Excellent resistance to Copper(II) Sulfate at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Potassium Permanganate CAS 7722-64-7 · KMnO4 | Excellent resistance to Potassium Permanganate at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Calcium Hydroxide (Hydrated Lime) CAS 1305-62-0 · CaH2O2 | Excellent resistance to Calcium Hydroxide (Hydrated Lime) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Sodium Lauryl Sulfate (SLS) CAS 151-21-3 · C12H25NaO4S | Good resistance to Sodium Lauryl Sulfate (SLS) at 20 °C; minor absorption or slight property shift possible over prolonged exposure or elevated temperature. | |
| Titanium Dioxide (TiO2) CAS 13463-67-7 · O2Ti | Excellent resistance to Titanium Dioxide (TiO2) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| Silicon Dioxide (Fumed Silica) CAS 7631-86-9 · O2Si | Excellent resistance to Silicon Dioxide (Fumed Silica) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. | |
| 1,4-Butanediol (BDO) CAS 110-63-4 · C4H10O2 | Excellent resistance to 1,4-Butanediol (BDO) at 20 °C with negligible swelling, weight change, or mechanical degradation in SAN. |
Source: Cole-Parmer / Thermo Scientific (Nalgene) / GF Piping Consensus · Retrieved 2026-11-25
Source SAN by Grade & Form Factor
Transparent SAN / UV-Stabilized · Injection & extrusion grades
View Suppliers on Made-in-China.comInjection molding & Extrusion manufacturers
View Suppliers on Made-in-China.com